SportMaster · Mixing procedure
Acrylic Patch Binder, 1-gallon batch
Job site recipe for a 1 gallon batch of patch mix: 1 gallon SportMaster Acrylic Patch Binder, 30 lbs clean silica sand (50–60 mesh) and 6 lbs Portland or Hydraulic Cement. Dry blend the sand and cement first until uniform; screening the cement to remove clumps is recommended. Slowly pour in the binder, stirring constantly, then keep mixing until a smooth, workable slurry forms, adjusting with small amounts of binder or sand. Mix only what can be applied within 30–60 minutes, and avoid adding water.
1 page, 3.9 MB
This is SportMaster's document, kept here so our customers and crews can read it beside our own pages. SportMaster's own copy is on sportmaster.net.
Open the PDF (1 page, 3.9 MB) Key facts
| Binder | 1 gallon SportMaster Acrylic Patch Binder |
|---|---|
| Sand | 30 lbs clean silica sand (50–60 mesh) |
| Cement | 6 lbs Portland or Hydraulic Cement (approx. ½ gallon dry volume) |
| Order | Dry blend sand and cement first, then add binder |
| Working time | Mix only what can be applied within 30–60 minutes |
| Water | Avoid adding water |
Taken from this document. The PDF is SportMaster's official document.
The full text of this document
This is the document's own text, moved from the PDF by machine, word for word, and checked against it. The PDF is SportMaster's official document. If the two ever differ, the PDF is right.
Job Site Mixing Instructions
SportMaster Acrylic Patch Binder – 1 Gallon Batch
Materials Needed:
- 1 gallon SportMaster Acrylic Patch Binder
- 30 lbs clean silica sand (50–60 mesh)
(Approx. 2 dry gallons or 26.74 lbs based on 13.37 lbs/gal)
- 6 lbs Portland or Hydraulic Cement
(Approx. ½ gallon dry volume)
Mixing Procedure:
1. Dry Blend First: In a clean mixing container, combine:
30 lbs Sand
6 lbs Cement
→ Mix thoroughly until uniform. Recommended: Screen cement to remove potential clumps before mixing.
2. Add Binder:
Slowly pour 1 gallon of Acrylic Patch Binder into the dry mix. Stir constantly while adding to prevent clumping.
3. Mix to Slurry:
Continue mixing until a smooth, workable slurry is formed. Adjust consistency as needed using small amounts of binder or sand.
Notes:
- Use clean tools and containers.
- Mix only what can be applied within 30 –60 minutes.
- Avoid adding water.
- Screening cement helps improve mix quality and prevent uneven texture.
Free estimates
Planning a court or a surface?
Industrial Surface is a SportMaster authorized installer in Northeast Ohio. Send the address and what you have in mind; we walk the site, measure it, and send a written proposal with the scope spelled out.
The yard
4000 East 86th Street, Cleveland, OH 44105
Off Broadway Avenue, south of downtown, ten minutes from I-77 and I-490.
Serving Cuyahoga, Summit, Lake, Lorain, Medina, Geauga, Portage, Stark and Ashtabula counties. Municipal, school, club, HOA and commercial work; residential courts by the job.